By Robin WenReviewed
Silicon Carbide Production: Zone by Zone
One Acheson run yields 15 to 19% saleable carbide. The core and the edge are different materials, because each impurity migrates its own way.

On this page
Silicon carbide production begins with a furnace that has no flame and no molten bath. A graphite core runs through a bed of quartz sand and carbon, current passes through the core until it glows, and the heat spreads outward through the charge. What comes out after the power is switched off is not one product. It is a series of zones, and the silicon carbide in the middle differs from the silicon carbide at the edge.
The economics are set by how much of that bed reacts at all. A 2019 thermodynamic study of the Acheson furnace puts commercial yields at low commercial yields of ∼15–19%
and power consumption at 7300−7600 kWh/t of product
. Everything else in the charge is either unreacted, partly reacted, or off-gas.
Silicon carbide production uses a resistor with a core, and the charge is a mixture
The Acheson furnace is a resistance heater whose element is the material being made. The study describes the construction as a central electrode in the form of a graphite core surrounded by a mixture of raw materials consisting of mainly a carbon source, silica sand and in some instances additives such as sawdust and sodium chloride
.
Silicon carbide production depends on each additive doing a mechanical job. Sawdust was added to improve gas permeability which in turn enhances the gas-solid reaction kinetics
, which matters because the reaction runs through the gas phase rather than through contact between grains. Salt was added to remove iron, aluminium, magnesium and calcium as volatile chlorides. That second job turned out not to work, and the section on it is further down.
The carbon source decides the cost, and it is also where most of the impurity budget enters. Petroleum coke is the clean option, coal is the cheap one, and the study notes the trade explicitly: low yields and high power consumption have pushed producers toward readily available low-purity raw materials, such as coal to reduce the cost of production
.
The reaction runs through a gas, and the product blocks itself
Silicon carbide does not form by silica touching carbon; it forms through silicon monoxide, and this is where silicon carbide production differs from a smelting reduction. The study lists the steps, and the third one is where the carbide appears:
SiO2(s) + C(s) → SiO(g) + CO(g)
2SiO2(l) + SiC(s) → 3SiO(g) + CO(g)
2C(s) + SiO(g) → SiC(s) + 2CO(g)The consequence of that mechanism is the reason the yield is low. Silicon carbide nucleates on the surface of the carbon grains, and the layer thickens: formation of SiC layers on C surface initiate at temperatures 1515–1530 °C
, and thickening of SiC layers restrict further reaction due to formation of a diffusion barrier
. A carbon grain that has been coated with silicon carbide is a grain that can no longer be reached, so the reaction stops while reactants remain.
The stages that follow are a temperature ladder. Silica melts at 1727 °C and starts wetting the carbon. Above 1800 °C the products are almost entirely gaseous. Above 2000 °C the silica in the hot zone is consumed and silicon carbide formation runs to completion — in that zone only. The outer charge stays below that temperature, which is why it leaves as partly reacted material.
Each impurity leaves the hot zone by its own route
The zones matter commercially because the impurities do not all accumulate in the same place. The study models the four main cationic impurities and finds four different outcomes:
| Impurity | Behaviour | Where it ends up |
|---|---|---|
| CaO, MgO | Evaporate as Ca(g) and Mg(g) below 2000 °C | Outer zone; least expected in the inner core zone |
| Al₂O₃ | Reduces to Al(g) and Al₂O(g), decomposing above 1900 °C | Reaction zone — aluminium stays where it is hottest |
| FeO | Reduces near 1500 °C, forms stable silicides | High-temperature zone |
| SiO₂ | Consumed above 2000 °C | Gone from the core, unreacted outside |
The first row is the useful one for a buyer. Calcium and magnesium leave the core and enrich the outer charge, so the crystalline silicon carbide from the centre of the furnace is the cleanest material the process produces — not because it was purified, but because the impurities migrated away from it. Aluminium and iron do the opposite and remain in or near the hot zone.
That is why the grade of the silicon carbide from an Acheson block depends on where in the block it came from, and why crushing and blending is a specification decision rather than a handling step. A supplier who blends the whole block has a consistent product; a supplier who sells the core separately has a different one.
Salt was the wrong answer, and the correction is recent
Adding sodium chloride to the charge was standard practice for decades, on the theory that it removed iron, aluminium, magnesium and calcium as gaseous chlorides. The study states the outcome without hedging: the practice was proved to be ineffective for the purification process
, citing a 2009 thermodynamic re-examination by Zhou and Telle, published in Materials Science Forum.
Two reasons are given for dropping it. The chlorides produced are hazardous, and the purification did not happen. What replaced it is not a better additive but a different strategy: the trend nowadays is aimed at harnessing the energy in the gaseous products
— recovering the carbon monoxide rather than trying to clean the charge.
The correction is worth noting because it is recent enough that older process descriptions still carry the salt step as if it worked.
Two American plants, one import line, and a fourth supplier
Supply is thinner than the process suggests. USGS records in its 2026 abrasives summary that crude silicon carbide was produced by two companies at two plants in 2025, with an estimated value of about $25 million, and that China supplied 97% of United States imports of crude silicon carbide and 57% of ground and refined material. A two-plant domestic industry and a single dominant import source is the whole supply picture for the abrasive grade.
Furnace or resynthesis: where the two routes part
Everything above describes metallurgical grade silicon carbide, which for the South African product the study cites means medium grade (82–88%SiC)
used as a reductant and deoxidant in steelmaking. The semiconductor and ceramic grades start from this material and then leave the Acheson route entirely: they are resynthesised from silicon and carbon, or grown from a vapour, and the resulting powder is specified by particle size and polytype rather than by position in a block.
The silicon carbide grade page covers those families and what each one is bought for, including the tariff split between loose grit and a sintered part. The production question is separate and narrower: what the furnace can deliver, and why 80% of what goes in does not become product.
What the process asks of a buyer
Three things follow from the zone structure:
- Which zone, and is it declared. Core material and blended material are different products with the same name. A certificate that gives a single SiC percentage is describing a blend.
- Which carbon source. The carbon sets the impurity budget before the furnace runs, and switching from coke to coal changes the product even at the same grade.
- Whether the CO is recovered. Power at 7,300–7,600 kWh per tonne and a yield below one fifth make the off-gas the difference between a viable plant and a marginal one.
Silicon production covers the neighbouring carbothermic process, where the same furnace logic applies to a metal rather than a carbide, and silicon carbide manufacturers covers who sells which form.
Methodology
Yield, energy consumption, temperatures, reaction steps and impurity behaviour are quoted from the 2019 Heliyon study cited below, which is a thermodynamic modelling exercise rather than a plant trial. Its impurity results are calculated equilibria, and the paper says so; they are reported here as the model’s conclusions, not as measurements from a specific furnace.
The grade description (82–88% SiC for the South African medium grade) is the study’s own characterisation of the local product, not a global figure. The reaction equations are reproduced as the study writes them, with the phase labels it uses.
Sources
- Matizamhuka, W.R., “Gas transport mechanisms and the behaviour of impurities in the Acheson furnace for the production of silicon carbide,” Heliyon 5(4), e01535 (2019) — furnace construction, sawdust and salt roles, 7300–7600 kWh/t, 15–19% yield, reaction steps and the diffusion barrier, impurity partitioning by zone, the Zhou and Telle correction on salt. https://pmc.ncbi.nlm.nih.gov/articles/PMC6479161/
- Zhou, L. and Telle, R., “Purifying mechanism in the Acheson process: a thermodynamic study,” Materials Science Forum 645–648, 41–44 (2010) — the re-examination that found salt addition ineffective, cited above as reported by Matizamhuka.
Related
- SpecificationSilicon Carbide: One Formula, Four GradesSilicon carbide is sold as grit, as a sintered ceramic and as a wafer. The numbers that identify each are not the same numbers.
- UsesSilicon Carbide Uses: Grit, Parts, WafersAbrasives, kiln furniture and power-device substrates buy the same compound. Three separate markets, three specs, and no route between them.
- SuppliersSilicon Carbide Manufacturers: Two FormsSilicon carbide manufacturers and suppliers split into two chains: abrasive grit sold by the tonne, and substrates sold by the wafer.
- Silicon · Critical MineralsSilicon Production: Purity Leaves the SolidA carbon furnace stops at 98% because boron arrives with the quartz and survives the solid. Purity is reached by changing the molecule.