By Robin WenReviewed

Bismuth Production: Two Unlike Routes

Kroll-Betterton and Betts are alternatives, not stages. Both reach four nines, and the intermediates between bullion and metal are not the same material.

A close view of bismuthinite, dark metallic bladed crystals in a matrix of white quartz and buff-coloured carbonate
Photo: Bismuthinite, the bismuth sulphide, in quartz; the ore mineral the traded metal almost never comes from · U.S. Geological Survey · Public domain · Wikimedia Commons · Cropped 396 px from the top and 397 px from the bottom to 5472x2855, then resized to 2400x1252; JPEG recompression
On this page

Bismuth production has two established routes, and they are alternatives. A lead refinery runs the Kroll-Betterton process or the Betts electrolytic process, not one after the other. Both start from lead bullion carrying bismuth as an impurity, and both end at four nines.

The Bureau of Mines described the pair in 1991, calling them the two most common methods of recovery, and that account is the one used here. It is also a snapshot: the process descriptions are still how these routes work, and the capacity figures beside them are from 1990.

RouteWhere the bismuth separatesEndpoint
Kroll-BettertonA dross skimmed off molten bullion99.99%
BettsAnode slime from electrolysis99.995%

The pyrometallurgical route

Kroll-Betterton adds calcium and magnesium to molten lead held at 485 °C. The two metals combine with bismuth into insoluble compounds that are lighter than lead, so they rise and can be skimmed off as a dross. The bullion leaves cleaner and the dross leaves carrying the bismuth.

The dross is the feed to the rest of this bismuth production route, which is short. It is treated first with chlorine or lead chloride and then with caustic soda to remove the calcium, magnesium, and remaining lead, and what remains is at 99.99% purity.

The report gives those two reagents as one treatment, not two jobs: the purification on this route is entirely chemical, and it does not say which reagent takes which impurity. The report calls this step a pyrometallurgical separation and treatment of the dross, which is as far as it characterises the route.

At the time, this was the only one currently used in the domestic lead industry, which made the American supply a single refinery’s dross line. Bismuth covers what a supply concentrated that way did to the price in 2025.

The electrolytic route

Betts treats bullion that is at least 90% lead. The bullion is cast into anodes, pure lead sheets hang between them, and the electrolyte is lead fluorosilicate with fluosilicic acid and a little glue to keep the cathode deposit coherent. Lead dissolves from the anode and plates onto the cathode.

The metal does not follow. Bismuth, copper, and other metals do not transfer to the cathode, but form anode slimes, which are collected, washed, and remelted to produce slag.

The slag then has to be reduced. It is mixed with sulfur and reduced with carbon, which gives a copper matte and a metal containing 20% to 25% bismuth. That crude metal is refined with caustic soda and nitrite to 99.995%.

The report adds a line that matters when reading capacity tables: The Betts process is common in foreign bismuth production.

The two intermediates are different materials

The two endpoints sit within 0.005 of each other, and the intermediates do not resemble each other at all.

Kroll-BettertonBetts
SeparationIntermetallic compound, floatsBismuth does not plate at the cathode
IntermediateDross, to reagent treatmentSlag, reduced to matte; crude metal at 20–25%
Treatment after separationChlorine or lead chloride, then caustic sodaCaustic soda and nitrite
Equipment impliedChlorination and caustic line beside a lead kettleCell house, matte smelter, refining kettle
Endpoint99.99%99.995%
  • Pyrometallurgical — Kroll-Betterton: dross, reagent treatment, no current.
  • Electrolytic — Betts: anode slime, matte reduction, caustic refining.
  • Both — four nines at the end, from lead bullion at the start.

A dross and a crude metal at 20% to 25% bismuth are different feed materials, and the report describes different equipment for each. What it does not give is a bismuth content for the dross, so the two intermediate grades cannot be put on one scale — the column above says what each intermediate is, not how they rank.

The step in bismuth production that cannot travel

Neither route takes bismuth as it occurs, as the USGS summary makes clear when it notes that no bismuth is mined for its own sake. Kroll-Betterton and Betts both begin with lead bullion, which means a copper smelter cannot finish the job no matter how much bismuth arrives in its feed: copper smelting concentrates bismuth into flue dust and anode slime, and the recovery only happens once that material reaches a lead smelter.

What leavesWhere it comes fromWhere it must go
Copper flue dustCopper smelterA lead smelter
Copper anode slime drossCopper refineryA lead smelter

This is the step that makes the logistics a cost item rather than a routing detail. What travels is a low-concentration intermediate, not metal — a tonne of flue dust carries a small fraction of a tonne of the metal, so the freight is paid on material that is mostly not the product.

The constraint has a geographic consequence. The report these figures come from describes American copper dust going to American lead smelters, and the United States has had no primary lead smelter since the end of 2013. The upstream step still exists; the destination no longer does.

Bismuth has its own minerals, and they are not the feedstock

Bismuthite, bismuthinite and bismutite are the minerals a report would name, and the same report is explicit that they usually do not constitute ore bodies worked for bismuth alone. That is the premise both routes depend on: the metal arrives as a by-product of lead, tungsten or zinc, which is why every process above starts from somebody else’s bullion. It also explains where the finished metal goes — a large share ends up in aluminum castings, in free-machining steel and in medical and cosmetic preparations, applications where a few tenths of a percent of the metal changes how the material behaves.

What to ask before specifying a bismuth route

  1. Which of the two routes the plant runs. They are alternatives, and the intermediates they produce are different materials.
  2. Whether the number on the supplier’s sheet describes the endpoint or the feed. 99.99% and 99.995% are close; a dross and a crude metal at 20–25% are not the same thing.
  3. Where any copper-route material goes. If it leaves the country for a lead smelter, the bismuth content is not local production.
  4. The vintage of any capacity figure. The table in the 1991 report is dated 31 December 1990.
  5. Whether the feed is primary or secondary. A reprocessed fusible alloy has already been through a refinery once; western lead ore carrying bismuth runs from 0.35% to 2.0%.

Methodology

The two routes, the 485 °C bullion temperature, the dross treatment and its reagents, the 99.99% and 99.995% endpoints, the Betts cell chemistry and its 90% lead feed requirement, the crude metal at 20% to 25%, the copper flue-dust and slime handling, the Australian concentrate movements, the Anaconda and Warrego figures, the scrap export destination, the three bismuth minerals, the western ore range and the Missouri note all come from U.S. Bureau of Mines Information Circular 9312, published in 1991 and describing the industry at the end of 1990.

The capacity table, the company names and the reserve figures in that report are historical and are not carried forward. Where the two sources disagree on dates, the page says so instead of picking one: the 1979 and 1996 dates for Bolivia describe different events, a production stop and a mine closure, and the report’s statement that Tasna was still producing copper and tin in 1991 fits both. The current market picture is in bismuth and the companies in bismuth suppliers.

Sources

  1. Stephen M. Jasinski, Bismuth—Uses, Supply, and Technology, U.S. Bureau of Mines Information Circular 9312, 1991 (recovery technology, both routes, purity endpoints, copper and secondary handling, mineral sources). https://stacks.cdc.gov/view/cdc/235669/cdc_235669_DS1.pdf
  2. U.S. Geological Survey, Mineral Commodity Summaries 2026: Bismuth, February 2026 (closure of the last American primary lead smelter, current byproduct sources, Tasna inactivity). https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-bismuth.pdf
Share: